SE25 - jacobHpayne/thermo-driver GitHub Wiki
Slumping Experiment 2025
Full Cycle
Sample: 120 x 100 x 1.1 mm Corning Eagle Glass
Dwell Temperatures (ºC): 730, 745, 760, 775, 790
Dwell durations (hours): 36, 78, 120
Sample Identification
ID | Material | Dwell Temp (ºC) | Dwell Duration (hrs) | Start | End | Status | Location |
---|---|---|---|---|---|---|---|
SE25-1 | 120x100x1.1 mm glass | 760 | 36 | 2025-02-01 | 2025-02-06 | Measured | VAN 611 |
SE25-2 | 120x100x1.1 mm glass | 760 | 78 | 2025-02-08 | 2025-02-14 | Measured | VAN 611 |
SE25-3 | 120x100x1.1 mm glass | 760 | 120 | 2025-02-15 | 2025-02-23 | Measured | VAN 611 |
SE25-4 | 120x100x1.1 mm glass | 745 | 36 | 2025-02-24 | 2025-02-28 | Measured, cut | VAN 611 |
SE25-5 | 120x100x1.1 mm glass | 745 | 78 | 2025-03-10 | 2025-03-16 | Measured, coating removed from edges | VAN 611 |
SE25-6 | 120x100x1.1 mm glass | 745 | 120 | 2025-03-18 | 2025-03-26 | Measured | VAN 611 |
SE25-7 | 120x100x1.1 mm glass | 730 | 36 | 2025-03-26 | 2025-03-31 | Slumped | VAN B11 |
SE25-8 | 120x100x1.1 mm glass | 775 | 36 | 2025-03-31 | 2025-04-05 | Slumped | VAN B11 |
SE25-9 | 120x100x1.1 mm glass | 790 | 36 | 2025-04-07 | 2025-04-12 | Slump Failed, Furnace Aborted - Temp Record | B11 Storage Demo |
SE25-10 | 120x100x1.1 mm glass | 730 | 78 | 2025-04-22 | 2025-04-28 | Slumped | VAN B11 |
SE25-11 | 120x100x1.1 mm glass | 730 | 120 | 2025-04-28 | 2025-05-06 | Slumped | VAN B11 |